②原料技術(shù)數(shù)據(jù)性能項目試驗條件[狀態(tài)]測試方法測試數(shù)據(jù)數(shù)據(jù)單位基本性能24小時吸水率---ASTMD-5700.6%物理性能泰伯磨耗量CS-17輪ASTMD-10443mg/1000rev比重---ASTMD-7921.17---熔體流動速率---ASTMD-12385.3g/10min泰伯磨耗量H18輪ASTMD-1044100mg/1000rev
機械性能硬度計硬度---ASTMD-224040---揉曲模量23℃ASTMD-79062MPa斷裂拉伸力---ASTMD-63828MPa斷裂伸長---ASTMD-638550%拉伸力5%伸長10%伸長---ASTMD-638ASTMD-6382.43.6MPaMPa埃佐沖擊強度23℃ASTMD-256不破裂J/m初耐撕裂性能---ASTMD-1004101kn/m熱性能熔點---ASTMD-3418150℃維卡軟化點---ASTMD-1525108℃熱畸變溫度@0.5MPaASTMD-64854℃熱畸變溫度@0.18MPaASTMD-648N/A℃其它性能耐揉曲切口增長性能---ASTMD-1052 1 106---